| Nozzle temperature | 250 °C | SpoolmanDB filaments/bambulab.json, object '{color_name}' (PC); kept beside the Open Filament Database value because they differ or the OFD entry lacks it; single starting extruder temperature (CONTRIBUTING.md: the temperature to start at that works in most cases), degrees Celsius per README.md | claim | github.com 2026-11-16“"extruder_temp": 250” |
|---|
| 260 to 280 °C | recommended nozzle temperature range (OFD fields min_print_temperature to max_print_temperature; unit per OFD schemas/filament_schema.json) | claim | github.com 2026-11-16“"min_print_temperature": 260, "max_print_temperature": 280” |
| Bed temperature | 90 to 110 °C | recommended bed temperature range (OFD fields min_bed_temperature to max_bed_temperature; unit per OFD schemas/filament_schema.json); SpoolmanDB filaments/bambulab.json line 1563 is consistent (100 °C) | claim | github.com 2026-11-16“"min_bed_temperature": 90, "max_bed_temperature": 110” |
|---|
| Density | 1.2 g/cm3 | OFD field density, g/cm³ per schemas/filament_schema.json; SpoolmanDB filaments/bambulab.json line 1563 gives the same density | claim | github.com 2026-11-16“"density": 1.2” |
|---|
| Tensile strength | 55 MPa | XY print direction; ISO 527, GB/T 1040; plus or minus 4 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "tensile_strength", "direction": "XY", "value": 55, "plus_minus": 4, "unit": "MPa"” |
|---|
| 34 MPa | Z print direction; ISO 527, GB/T 1040; plus or minus 3 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "tensile_strength", "direction": "Z", "value": 34, "plus_minus": 3, "unit": "MPa"” |
| Young's modulus | 2110 MPa | XY print direction; ISO 527, GB/T 1040; plus or minus 40 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "tensile_modulus", "direction": "XY", "value": 2110, "plus_minus": 40, "unit": "MPa"” |
|---|
| 1450 MPa | Z print direction; ISO 527, GB/T 1040; plus or minus 60 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "tensile_modulus", "direction": "Z", "value": 1450, "plus_minus": 60, "unit": "MPa"” |
| Elongation at break | 3.8 % | XY print direction; ISO 527, GB/T 1040; plus or minus 0.3 %; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "elongation_at_break", "direction": "XY", "value": 3.8, "plus_minus": 0.3, "unit": "%"” |
|---|
| 2.1 % | Z print direction; ISO 527, GB/T 1040; plus or minus 0.4 %; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "elongation_at_break", "direction": "Z", "value": 2.1, "plus_minus": 0.4, "unit": "%"” |
| Heat deflection temp. | 112 °C | HDT at 0.45 MPa load; ISO 75 0.45 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "heat_deflection_045", "direction": "unknown", "value": 112, "unit": "°C"” |
|---|
| 117 °C | HDT at 1.8 MPa load; ISO 75 1.8 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "heat_deflection_18", "direction": "unknown", "value": 117, "unit": "°C"” |
| Diameter tolerance | 0.03 mm | plus or minus, on the filament diameter (OFD field diameter_tolerance, mm per schemas/filament_schema.json; 0.02 is the schema default and is not taken) | claim | github.com 2026-11-16“"diameter_tolerance": 0.03” |
|---|
| Drying temperature | 80 °C | recommended drying temperature (OFD field dry_temperature; unit per OFD schemas/filament_schema.json) | claim | github.com 2026-11-16“"dry_temperature": 80” |
|---|
| Drying time | 8 h | recommended drying time at the drying temperature (OFD field dry_time, hours per schemas/filament_schema.json) | claim | github.com 2026-11-16“"dry_time": 8” |
|---|
| Filament diameter | 1.75 mm | offered filament diameter (sizes.json field diameter, mm per schemas/sizes_schema.json); first seen in colour variant black | claim | github.com 2026-11-16“"diameter": 1.75” |
|---|
| Flexural modulus | 2310 MPa = 2.31 GPa | XY print direction; ISO 178, GB/T 9341; plus or minus 70 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "flexural_modulus", "direction": "XY", "value": 2310, "plus_minus": 70, "unit": "MPa"” |
|---|
| 1620 MPa = 1.62 GPa | Z print direction; ISO 178, GB/T 9341; plus or minus 80 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "flexural_modulus", "direction": "Z", "value": 1620, "plus_minus": 80, "unit": "MPa"” |
| Flexural strength | 108 MPa | XY print direction; ISO 178, GB/T 9341; plus or minus 4 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "flexural_strength", "direction": "XY", "value": 108, "plus_minus": 4, "unit": "MPa"” |
|---|
| 55 MPa | Z print direction; ISO 178, GB/T 9341; plus or minus 2 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "flexural_strength", "direction": "Z", "value": 55, "plus_minus": 2, "unit": "MPa"” |
| Impact strength | 34.8 kJ/m2 | XY print direction; ISO 179, GB/T 1043; plus or minus 2.1 kJ/m2; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "impact_strength", "direction": "XY", "value": 34.8, "plus_minus": 2.1, "unit": "kJ/m2"” |
|---|
| 9.0 kJ/m2 | Z print direction; ISO 179, GB/T 1043; plus or minus 0.4 kJ/m2; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "impact_strength", "direction": "Z", "value": 9.0, "plus_minus": 0.4, "unit": "kJ/m2"” |
| Impact strength notched | 7.5 kJ/m2 | notched; XY print direction; ISO 179, GB/T 1043; plus or minus 1.3 kJ/m2; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "impact_strength_notched", "direction": "XY", "value": 7.5, "plus_minus": 1.3, "unit": "kJ/m2"” |
|---|
| Spool net mass | 1000 g = 1 kg | offered net filament weight per spool (sizes.json field filament_weight, grams per schemas/sizes_schema.json); first seen in colour variant black | claim | github.com 2026-11-16“"filament_weight": 1000” |
|---|
| Vicat softening temperature | 119 °C | ISO 306, GB/T 1633; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://cdn.shopify.com/s/files/1/0645/5876/0155/files/Bambu_PC_Technical_Data_Sheet.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "vicat_softening", "direction": "unknown", "value": 119, "unit": "°C"” |
|---|