Key specifications
| Nozzle temperature | 260 to 290 °C source |
|---|---|
| Bed temperature | 80 to 100 °C source |
| Density | 1.29 g/cm³ source |
| Tensile strength | 74 MPa, 35 MPa 2 sources |
| Young's modulus | 4,730 MPa, 2,160 MPa 2 sources |
| Elongation at break | 4.5 %, 2.4 % 2 sources |
| Heat deflection temp. | 182 °C, 205 °C 2 sources |
Specifications
| Attribute | Value | Conditions | Type | Source, read date, quote |
|---|---|---|---|---|
| Nozzle temperature | 260 to 290 °C | recommended nozzle temperature range (OFD fields min_print_temperature to max_print_temperature; unit per OFD schemas/filament_schema.json); SpoolmanDB filaments/bambulab.json line 2049 is consistent (270 °C) | claim | github.com 2026-11-16“"min_print_temperature": 260, "max_print_temperature": 290” |
| Bed temperature | 80 to 100 °C | recommended bed temperature range (OFD fields min_bed_temperature to max_bed_temperature; unit per OFD schemas/filament_schema.json); SpoolmanDB filaments/bambulab.json line 2049 is consistent (90 °C) | claim | github.com 2026-11-16“"min_bed_temperature": 80, "max_bed_temperature": 100” |
| Density | 1.29 g/cm3 | OFD field density, g/cm³ per schemas/filament_schema.json; SpoolmanDB filaments/bambulab.json line 2049 gives the same density | claim | github.com 2026-11-16“"density": 1.29” |
| Tensile strength | 74 MPa | XY print direction; ISO 527, GB/T 1040; plus or minus 6 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "tensile_strength", "direction": "XY", "value": 74, "plus_minus": 6, "unit": "MPa"” |
| 35 MPa | Z print direction; ISO 527, GB/T 1040; plus or minus 5 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "tensile_strength", "direction": "Z", "value": 35, "plus_minus": 5, "unit": "MPa"” | |
| Young's modulus | 4730 MPa | XY print direction; ISO 527, GB/T 1040; plus or minus 260 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "tensile_modulus", "direction": "XY", "value": 4730, "plus_minus": 260, "unit": "MPa"” |
| 2160 MPa | Z print direction; ISO 527, GB/T 1040; plus or minus 170 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "tensile_modulus", "direction": "Z", "value": 2160, "plus_minus": 170, "unit": "MPa"” | |
| Elongation at break | 4.5 % | XY print direction; ISO 527, GB/T 1040; plus or minus 1.2 %; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "elongation_at_break", "direction": "XY", "value": 4.5, "plus_minus": 1.2, "unit": "%"” |
| 2.4 % | Z print direction; ISO 527, GB/T 1040; plus or minus 0.8 %; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "elongation_at_break", "direction": "Z", "value": 2.4, "plus_minus": 0.8, "unit": "%"” | |
| Heat deflection temp. | 205 °C | HDT at 0.45 MPa load; ISO 75 0.45 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "heat_deflection_045", "direction": "unknown", "value": 205, "unit": "°C"” |
| 182 °C | HDT at 1.8 MPa load; ISO 75 1.8 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "heat_deflection_18", "direction": "unknown", "value": 182, "unit": "°C"” | |
| Diameter tolerance | 0.03 mm | plus or minus, on the filament diameter (OFD field diameter_tolerance, mm per schemas/filament_schema.json; 0.02 is the schema default and is not taken) | claim | github.com 2026-11-16“"diameter_tolerance": 0.03” |
| Drying temperature | 80 °C | recommended drying temperature (OFD field dry_temperature; unit per OFD schemas/filament_schema.json) | claim | github.com 2026-11-16“"dry_temperature": 80” |
| Filament diameter | 1.75 mm | offered filament diameter (sizes.json field diameter, mm per schemas/sizes_schema.json); first seen in colour variant black | claim | github.com 2026-11-16“"diameter": 1.75” |
| Flexural modulus | 5320 MPa = 5.32 GPa | XY print direction; ISO 178, GB/T 9341; plus or minus 270 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "flexural_modulus", "direction": "XY", "value": 5320, "plus_minus": 270, "unit": "MPa"” |
| 2210 MPa = 2.21 GPa | Z print direction; ISO 178, GB/T 9341; plus or minus 180 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "flexural_modulus", "direction": "Z", "value": 2210, "plus_minus": 180, "unit": "MPa"” | |
| Flexural strength | 131 MPa | XY print direction; ISO 178, GB/T 9341; plus or minus 6 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "flexural_strength", "direction": "XY", "value": 131, "plus_minus": 6, "unit": "MPa"” |
| 49 MPa | Z print direction; ISO 178, GB/T 9341; plus or minus 5 MPa; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "flexural_strength", "direction": "Z", "value": 49, "plus_minus": 5, "unit": "MPa"” | |
| Impact strength | 36.0 kJ/m2 | XY print direction; ISO 179, GB/T 1043; plus or minus 2.7 kJ/m2; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "impact_strength", "direction": "XY", "value": 36.0, "plus_minus": 2.7, "unit": "kJ/m2"” |
| 4.5 kJ/m2 | Z print direction; ISO 179, GB/T 1043; plus or minus 0.6 kJ/m2; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "impact_strength", "direction": "Z", "value": 4.5, "plus_minus": 0.6, "unit": "kJ/m2"” | |
| Impact strength notched | 8.6 kJ/m2 | notched; XY print direction; ISO 179, GB/T 1043; plus or minus 0.5 kJ/m2; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "impact_strength_notched", "direction": "XY", "value": 8.6, "plus_minus": 0.5, "unit": "kJ/m2"” |
| Spool net mass | 500 g = 0.5 kg | offered net filament weight per spool (sizes.json field filament_weight, grams per schemas/sizes_schema.json); first seen in colour variant black | claim | github.com 2026-11-16“"filament_weight": 500” |
| 1000 g = 1 kg | offered net filament weight per spool (sizes.json field filament_weight, grams per schemas/sizes_schema.json); first seen in colour variant black | claim | github.com 2026-11-16“"filament_weight": 1000” | |
| Vicat softening temperature | 226 °C | ISO 306, GB/T 1633; printed specimen, 100% infill; annealed and dried at 80 °C for 12 h; from the brand's data sheet https://store.bblcdn.com/9690d6226f024acab2ba0dd52dabb654.pdf (primary source, read by OFD contributors 2026-11-08) | spec | github.com 2026-11-16“"property": "vicat_softening", "direction": "unknown", "value": 226, "unit": "°C"” |
Variations from this maker